Almost every print defect has a recognisable look. If you can classify it, you find the cause quickly. The table summarises the most frequent cases in FDM.
| What you see | Likely cause | Remedy |
|---|---|---|
| Corners lift off the plate (warping) | material shrinks, adhesion too weak | clean the plate, raise bed temperature, add a brim, avoid draughts, use an enclosure |
| Fine strings between parts (stringing) | material oozes during travel moves | increase retraction, lower temperature, dry the filament |
| Layers shifted sideways | loose belt, collision, acceleration too high | tension the belts, reduce speed |
| Gaps, thin lines (under-extrusion) | partly clogged nozzle, temperature too low, damp filament | clean the nozzle, raise temperature, dry the filament |
| First layer does not stick | wrong nozzle distance, greasy plate | reset the distance, clean with isopropanol |
| First layer too wide (elephant's foot) | nozzle too close, bed too hot | increase the distance, compensate in the slicer |
| Layers separate | printed too cold, too much cooling | raise temperature, reduce fan |
| Ripples beside edges (ghosting) | vibration at fast direction changes | lower acceleration, use vibration compensation |
| Sagging overhangs | too steep, too warm, too little cooling | supports, more cooling, different orientation |
| Bubbles and crackling | damp filament | dry it |
| Holes in the top face | too few top layers, infill too sparse | add top layers |
| Visible seam | start point of each layer | place the seam in an edge |
The three most common roots
The first layer. A large share of failed prints go wrong in the first minutes. A clean, correctly set build plate solves most adhesion problems.
Damp filament. PETG, TPU and nylon take up water from the air. The result is strings, bubbles and weak parts. Drying in a filament dryer or an oven at low temperature helps.
Expecting too much speed. Fast profiles amplify almost every defect. When there are problems, slow down first.
Work systematically
- Photograph and classify the defect.
- Change one setting only.
- Check with a small test part, not the big print.
- Save working settings as a profile.
Defects in resin prints
- Part comes off the platform: first-layer exposure too short or platform not level
- Missing areas: too few supports, suction in hollow parts without a drain hole
- Sticky surface: insufficient washing or post-curing
- Cracks after a few days: liquid resin trapped in cavities
FAQ
Why does the same print sometimes fail?
Room temperature, draughts, filament moisture and plate contamination change from day to day. Constant conditions give constant results.
How often does a printer need maintenance?
Clean the plate before every print, change the nozzle when needed, check guides and belts every few months. Modern machines largely calibrate themselves.
Our own service: If a part will not work at home, 3D Druck Berlin prints it for you, including in materials open machines cannot handle: upload a file for an instant quote.
More topics
- Design rulesGuide values for walls, overhangs, holes, lettering and joints.
- Tolerances and fitsWhat accuracy is realistic and how to design fits.
- Slicer settingsWhich setting does what, and where to start.
- Post-processingFrom raw print to finished part: sanding, painting, gluing, inserts.
- CAD programsFrom browser building blocks to parametric CAD: what suits whom.
- 3D scanningPhotogrammetry, structured light, laser: what a scan delivers and where it ends.
- The first printFrom unboxing to the first successful part.
- Buying a 3D printerDesigns, features, price classes and running costs, without brand advertising.
- Finding modelsWhere ready-made 3D models are and how to spot good ones.